TABLE 9

 
 

CHEMICAL COMPOSITION LIMITS FOR 2XXX SERIES
WROUGHT ALUMINUM ALLOYS

 
 
 

Alloy

Silicon

Iron

Copper

Manganese

Magnesium

Chromium

Nickel

Zinc

Titanium

Others

Aluminum

Each

Total

 

min

max

max

min

max

min

max

min

max

min

max

min

max

max

max

min

max

 

2011

 

.40

.70

5.0

6.0

               

.30

 

.05

.15

Remainder

2014

.50

1.2

1.0

3.9

5.0

.40

1.2

.20

.80

 

.10

   

.25

 

.05

.15

Remainder

2017

 

.80

1.0

3.5

4.5

.40

1.0

.20

.80

 

.10

   

.10

 

.05

.15

Remainder

2018

 

.90

1.0

3.5

4.5

 

.20

.45

.90

 

.10

1.7

2.3

.25

 

.05

.15

Remainder

2024

 

.50

.50

3.8

4.9

.30

.90

1.2

1.8

 

.10

   

.10

 

.05

.15

Remainder

Alclad 2024

2024 Alloy Sheet Clad Both Sides with 99.3 Alloy

2025

.50

1.2

1.0

3.9

5.0

.40

1.2

 

.05

 

.10

   

.25

.15

.05

.15

Remainder

2117

 

.80

1.0

2.0

3.0

 

.20

.20

.50

 

.10

   

.10

 

.05

.15

Remainder

2218

 

.90

1.0

3.5

4.5

 

.20

1.2

1.8

 

.10

1.7

2.3

.25

 

.05

.15

Remainder

 
 
Available Through Authorized Sanford Licensees
 
 
SANFORD PROCESS™ CORPORATION
1 Shorr Court, Woonsocket, RI 02895
Tel: (401) 597-5000 Fax: (401) 597-5485
Owners of Patents of the World's Finest Hard Anodized Process

 

 

 
 
 
Copyright © 2000 Sanford Process
Site designed by WorldWideWebWorks
 
 
 

 

   Katahdin
61 North Avenue Natick, MA 01760       T:508-653-7900
©2011